Materials guide · High-performance

How to 3D print PEEK

PEEK is the reference high-performance thermoplastic: semi-crystalline, chemically resistant and rated for continuous use around 250 °C. It is also the hardest of the common polymers to print well. This guide covers typical settings, the amorphous-print-then-anneal route, and an honest view of what an Epitum printer can do with it.

What PEEK is — and when to choose it

Polyether ether ketone (PEEK) belongs to the PAEK family. Its melting point sits around 340 °C and its glass transition near 145–150 °C. Fully crystallized, it keeps its stiffness well above that, resists almost every solvent, fuel and hydraulic fluid, and is inherently flame-retardant. It is specified for aerospace brackets, oil-and-gas seals, semiconductor fixtures and medical devices.

The same crystallinity makes printing hard. PEEK crystallizes fast as it cools; a cold layer shrinks and stops bonding to the next one. Many dedicated PEEK machines fight this with build environments of 150–200 °C; others run 90–100 °C chambers and rely on annealing. If you only need chemical and heat resistance, PPS carbon fiber prints far more easily. If you need PAEK-class performance with a wider process window, look at PEKK, or at amorphous PEI when a 170–200 °C service ceiling is enough.

Typical properties

PropertyTypical rangeTest method
Glass transition (Tg)143–152 °CISO 11357 (DSC)
Melting point (Tm)338–343 °CISO 11357 (DSC)
Tensile modulus, XY3.0–4.0 GPaISO 527
Tensile yield strength, XY60–95 MPaISO 527
Tensile strength, Z (through layers)20–85 MPa — highly process-dependentISO 527
HDT at 1.8 MPa (not annealed)≈ 150 °CISO 75
Continuous use temperature (crystallized)≈ 250–260 °CManufacturer rating
Density≈ 1.30 g/cm³ISO 1183
Flammability (base resin)UL94 V-0UL94

Typical published values across manufacturers, measured on test specimens; check your spool’s datasheet. Printed parts are usually weaker between layers (Z) than along them (XY).

The spread in through-layer (Z) strength is the real story. One maker publishes anywhere from 20 to 85 MPa for the same filament, depending only on process conditions.

Typical print settings

Nozzle temperature380–420 °C (Epitum: up to 430 °C)
Build plate120–160 °C (Epitum: up to 150 °C)
Chamber70–140 °C for amorphous printing; ≥ 150 °C to crystallize in the printer (Epitum: up to 90 °C)
Print speed20–40 mm/s
Part coolingOff
Drying120 °C · 4–5 h (moisture < 0.02 %); lower and longer if the spool is not rated for it
Nozzle430 °C-rated, ≥ 0.4 mm; hardened for filled grades

Starting point compiled from manufacturers’ recommendations — fine-tune with the Printoformer material profile for your spool, nozzle and part geometry.

The Epitum hot end reaches 430 °C, which covers the typical PEEK nozzle range. The limit is the chamber. Epitum heats its chamber actively to 90 °C, while semi-crystalline-as-printed PEEK wants roughly 150 °C. In practice that means the amorphous route that filament makers publish for cooler printers: a chamber below 150 °C (one PAEK maker's example profile uses 60 °C), then a separate anneal. You print PEEK largely amorphous, getting good layer fusion, a translucent amber-brown look, and lower stiffness and chemical resistance. Then you anneal the part to crystallize it.

Which Epitum: JL or L

For PEEK we usually suggest the Epitum L. It is a single-material job, and the 360 × 360 × 610 mm volume is rarely the constraint; part size is limited by warping, not by the frame. The Epitum JL makes sense if you want a nozzle dedicated to PEEK, or need a second material. Soluble supports for the PAEK class do exist, but they are specialized high-temperature products; see the general soluble-support guide. We don't promise PEEK results without seeing the part. We evaluate each part's geometry, size and load case individually.

Applications

  • Small brackets, clips and housings for hot or chemically aggressive environments
  • Pump, valve and fluid-handling components exposed to fuels and solvents
  • Electrical insulators and fixtures that must hold shape near 200 °C after annealing
  • Prototypes and short runs of parts later machined or molded in PEEK

Troubleshooting and tips

  • Keep parts compact. Warping and interlayer delamination grow with footprint and height. Start small, use generous brims, and avoid long thin walls and sharp corners.
  • Control drafts. Keep the chamber closed and preheated before the first layer, and do not open the door mid-job. A cold draft on one side shows up as a crack between layers.
  • Bed adhesion. Typical surfaces are PEI sheet, polyimide (Kapton-type) tape or a high-temperature adhesive made for PAEK. Let the plate cool before removal.
  • Dry, then print from a heated box. PEEK absorbs little water, but traces at 400 °C cause bubbles and stringing.
  • Anneal with support. Published schedules ramp slowly (about 3 °C/min) to roughly 170–200 °C, hold 2–4 h, then cool slowly. Parts shrink slightly and can distort, and no maker gives a universal figure. Support thin features in a fixture or sand bed, and measure a test part first. Opaque beige means it worked.

Not in our standard catalog. Talk to an engineer about your PEEK part: contact us →

Frequently asked questions

Can you 3D print PEEK with a 90 °C chamber?

Yes, for small and medium parts, by printing it largely amorphous and annealing afterwards — the route PEEK makers publish for cooler printers. Large or tall parts carry a rising risk of warping and layer separation; machines with 150 °C+ build environments handle those better. Send us the part and we will tell you which side of the line it falls on.

Why is my printed PEEK amber and translucent?

Because it cooled before it could crystallize. Amorphous PEEK is translucent amber-brown. Annealing turns it opaque beige and restores stiffness, heat and chemical resistance.

What nozzle temperature does PEEK need?

Typically 380–420 °C across manufacturers. Epitum printers reach 430 °C, so the hot end is not the limit.

Is PEKK or PEI easier to print than PEEK?

Usually yes. PEKK crystallizes more slowly, so layers bond better. PEI is amorphous and needs no crystallization step, at the cost of a lower temperature ceiling.

Related guides

Keep reading

All material guides →

Talk to an engineer about your PEEK part

Send us the drawing, the load case and the service temperature — we will tell you honestly whether the Epitum envelope fits the part.

Talk to an engineer