How to 3D print polycarbonate (PC)

Polycarbonate is the tough, heat-resistant workhorse among unfilled engineering filaments — and one of the easiest to get wrong. This guide covers typical properties and settings across manufacturers, why it warps, why moisture matters, and when PC-ABS or ABS is the better choice.

$67.53 PC · 0.75 kg spool · USD
Order / Request a quote

What polycarbonate is — and when to choose it

Polycarbonate (PC) is an amorphous engineering thermoplastic known for impact toughness and for keeping its shape well above the point where ABS softens. Printed PC is chosen for functional housings, jigs and fixtures, brackets and covers that see heat or rough handling.

“PC filament” covers two families. Easy-print grades are modified to run at 250–275 °C and soften around 105–115 °C. Unmodified PC needs 280–310 °C and a 110–120 °C bed, but holds its shape to roughly 130–140 °C. Check which one your spool is before copying settings.

PC vs ABS vs PC-ABS: ABS prints cooler and warps less, but softens first. PC-ABS sits between them — easier to print and less notch-sensitive than PC, with less heat resistance. Pick PC when temperature or stiffness at temperature decides the part; for fire-rated enclosures see flame-retardant PC/ABS.

Typical properties

PropertyTypical rangeTest method
Tensile strength (printed, XY)45–70 MPaISO 527 / ASTM D638
Tensile modulus1.9–2.6 GPaISO 527 / ASTM D638
Elongation at break (XY)3–10%ISO 527 / ASTM D638
Notched Charpy impact4–12 kJ/m²ISO 179
Heat deflection, 0.45 MPa105–140 °C (higher for unmodified PC)ISO 75 / ASTM D648
Glass transition≈ 105–115 °C easy-print grades; ≈ 145–160 °C unmodifiedDSC / DMA
Density1.18–1.20 g/cm³ISO 1183 / ASTM D792

Typical published values across manufacturers, measured on test specimens; check your spool’s datasheet. Printed parts are usually weaker between layers (Z) than along them (XY).

Typical print settings

Nozzle temperature250–275 °C easy-print grades; 280–310 °C unmodified PC
Build plate90–120 °C; textured PEI (glue stick if needed) or polyimide tape
ChamberEnclosed; heated 70–100 °C for large parts (Epitum: up to 90 °C)
Print speed30–80 mm/s for strong parts; some grades are rated faster
Part coolingOff; low fan only for bridges
Drying75–80 °C · 6 h (easy-print) up to 120 °C · 4 h (unmodified) — per your TDS
NozzleBrass or hardened, ≥ 0.4 mm

Starting point compiled from manufacturers’ recommendations — fine-tune with the Printoformer material profile for your spool, nozzle and part geometry.

Dial in from the low end of your grade’s nozzle range and raise it 5 °C at a time until layers stop splitting. PC warps because it shrinks as it cools through its glass transition: the warmer and steadier the space around the part, the less stress builds up.

Which Epitum: JL or L

Both reach the temperatures PC needs: the 430 °C hot end covers even unmodified grades, and the actively heated chamber, up to 90 °C, sits inside the 70–100 °C band manufacturers recommend for large PC parts. The 360 × 360 × 610 mm volume is large enough that chamber heat is not optional for full-size parts.

The Epitum L suits single-material production of housings and fixtures. Choose the Epitum JL when the geometry needs support you cannot reach: its second nozzle prints soluble support for engineering plastics, and the mechanical valve that seals the idle nozzle means no wipe tower.

Applications

  • Jigs, fixtures and end-of-arm tooling that take impacts
  • Electronics housings and covers near warm components
  • Light guides and translucent covers, where clarity is not critical
  • Functional prototypes of injection-molded PC parts

Troubleshooting and tips

  • Bubbles, hissing, rough surface: the filament is wet. PC picks up moisture from the air and hydrolyzes at print temperature, which also costs strength. Dry it and print from a dry box.
  • Corners lifting: close the chamber, heat it, raise the bed, add a brim, and round sharp corners in CAD. Turn the part-cooling fan off.
  • Layer splitting on tall parts: too cold, too much fan or a cold chamber. Raise nozzle and chamber temperature before slowing down.
  • Cloudy “clear” parts: clear PC transmits light well as a solid, but layer lines and tiny voids scatter it. Prints come out translucent, not glass-clear; 100% infill, slower walls and polishing help.
  • Stress after printing: manufacturers suggest annealing, typically 90–100 °C for 2 h for easy-print grades, to relax internal stress.

Available from MG World Tech: PC, 0.75 kg spool, $67.53. Order or request a quote →

Frequently asked questions

What temperature do you print polycarbonate at?

Typically 250–310 °C at the nozzle. Easy-print, modified PC grades run at 250–275 °C; unmodified PC needs 280–310 °C with a 110–120 °C bed. The bed usually sits at 90–120 °C, with the fan off and an enclosed, heated chamber.

Do you need an enclosure to print PC?

Yes. Manufacturers call for an enclosure, and a heated chamber for large parts, because PC shrinks and warps as it cools. Epitum printers heat the chamber actively up to 90 °C.

Is polycarbonate stronger than ABS?

Generally yes: it is tougher, stiffer at temperature and keeps its shape well above where ABS softens. It is also harder to print — hotter, more warp-prone and more sensitive to moisture.

Can you 3D print clear polycarbonate?

Translucent, yes; optically clear, no. Clear PC transmits light well as a solid, but FFF layer lines and voids scatter it. Full infill, slow walls and post-polishing improve clarity.